{"id":1390,"date":"2018-07-10T22:00:00","date_gmt":"2018-07-10T20:00:00","guid":{"rendered":"https:\/\/new.rjl-microanalytic.de\/?p=1390"},"modified":"2023-06-04T15:45:07","modified_gmt":"2023-06-04T13:45:07","slug":"fehlerhafte-detektion-metallischer-partikel-durch-lichtmikroskopie","status":"publish","type":"post","link":"https:\/\/www.rjl-microanalytic.de\/en\/fehlerhafte-detektion-metallischer-partikel-durch-lichtmikroskopie\/","title":{"rendered":"Erroneous Detection of Metallic Particles by Light Microscopy"},"content":{"rendered":"<div data-elementor-type=\"wp-post\" data-elementor-id=\"1390\" class=\"elementor elementor-1390\" data-elementor-post-type=\"post\">\n\t\t\t\t\t\t<section class=\"elementor-section elementor-top-section elementor-element elementor-element-33b4a892 elementor-section-boxed elementor-section-height-default elementor-section-height-default\" data-id=\"33b4a892\" data-element_type=\"section\" data-e-type=\"section\">\n\t\t\t\t\t\t<div class=\"elementor-container elementor-column-gap-default\">\n\t\t\t\t\t<div class=\"elementor-column elementor-col-100 elementor-top-column elementor-element elementor-element-1cfb6989\" data-id=\"1cfb6989\" data-element_type=\"column\" data-e-type=\"column\" data-settings=\"{&quot;background_background&quot;:&quot;classic&quot;}\">\n\t\t\t<div class=\"elementor-widget-wrap elementor-element-populated\">\n\t\t\t\t\t\t<div class=\"elementor-element elementor-element-680ee604 elementor-widget elementor-widget-text-editor\" data-id=\"680ee604\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>The identification of metallic particles is an important requirement in cleanliness analysis. In recent years, the light-optical detection of metallic particles has commonly been performed by the means of gloss. On the basis of our laboratory experience, we have found that the light microscopic analysis often leads to incorrect typifications, which can be easily avoided by a material analysis using SEM-EDX.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-6fe3cc73 elementor-widget elementor-widget-heading\" data-id=\"6fe3cc73\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h3 class=\"elementor-heading-title elementor-size-default\">Light Microscopy Compared to SEM-EDX<\/h3>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-e28da8a elementor-widget elementor-widget-text-editor\" data-id=\"e28da8a\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>The light-microscopic detection of metallic particles is performed on the basis of light reflection. A particle is classified as metallic if it incorporates shiny spots. In all other cases, the particle is considered to be non-metallic. In\u00a0<a class=\"unterstrichen\" href=\"\/en\/analysenservice-mit-iso-17025-akkreditierung\/sem-edx-identifikation-partikelverunreinigungen\/\">SEM-EDX analysis.<\/a>\u00a0a particle's X-Ray spectrum is measured, allowing its elemental components to be identified. This information enables a precise material typification.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-10ad1054 elementor-widget elementor-widget-image\" data-id=\"10ad1054\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<img fetchpriority=\"high\" decoding=\"async\" width=\"1064\" height=\"332\" src=\"https:\/\/www.rjl-microanalytic.de\/wp-content\/uploads\/Metallisch-glaenzende-Partikel-SEM-EDX.jpg\" class=\"attachment-full size-full wp-image-2782\" alt=\"\" srcset=\"https:\/\/www.rjl-microanalytic.de\/wp-content\/uploads\/Metallisch-glaenzende-Partikel-SEM-EDX.jpg 1064w, https:\/\/www.rjl-microanalytic.de\/wp-content\/uploads\/Metallisch-glaenzende-Partikel-SEM-EDX-300x94.jpg 300w, https:\/\/www.rjl-microanalytic.de\/wp-content\/uploads\/Metallisch-glaenzende-Partikel-SEM-EDX-1024x320.jpg 1024w, https:\/\/www.rjl-microanalytic.de\/wp-content\/uploads\/Metallisch-glaenzende-Partikel-SEM-EDX-768x240.jpg 768w\" sizes=\"(max-width: 1064px) 100vw, 1064px\" \/>\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-6a8cf653 elementor-widget elementor-widget-heading\" data-id=\"6a8cf653\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h3 class=\"elementor-heading-title elementor-size-default\">Do Metallic Particles Really Shine?<\/h3>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-1363acf6 elementor-widget elementor-widget-text-editor\" data-id=\"1363acf6\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>The analysis of reflections requires that metals on a filter membrane actually shine. Since the contaminant particles are exposed to liquids, temperature and friction during component processing, their surface is often non-shiny, but dull or corroded. These metallic particles are erroneously classified as non-metallic by light microscopy. In the following example, three particles (zinc, steel and aluminum) are shown, which have been recognized by light microscopy as non-metallic. However, the SEM-EDX analysis shows the metallic nature of these particles.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-5c00e2d elementor-widget elementor-widget-image\" data-id=\"5c00e2d\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<a href=\"https:\/\/www.rjl-microanalytic.de\/wp-content\/uploads\/Nicht-glaenzende-Metalle-SEM-EDX.jpg\" data-elementor-open-lightbox=\"yes\" data-elementor-lightbox-title=\"Nicht-glaenzende-Metalle-SEM-EDX\" data-e-action-hash=\"#elementor-action%3Aaction%3Dlightbox%26settings%3DeyJpZCI6Mjc4MywidXJsIjoiaHR0cHM6XC9cL3d3dy5yamwtbWljcm9hbmFseXRpYy5kZVwvd3AtY29udGVudFwvdXBsb2Fkc1wvTmljaHQtZ2xhZW56ZW5kZS1NZXRhbGxlLVNFTS1FRFguanBnIn0%3D\">\n\t\t\t\t\t\t\t<img decoding=\"async\" width=\"992\" height=\"765\" src=\"https:\/\/www.rjl-microanalytic.de\/wp-content\/uploads\/Nicht-glaenzende-Metalle-SEM-EDX.jpg\" class=\"attachment-full size-full wp-image-2783\" alt=\"\" srcset=\"https:\/\/www.rjl-microanalytic.de\/wp-content\/uploads\/Nicht-glaenzende-Metalle-SEM-EDX.jpg 992w, https:\/\/www.rjl-microanalytic.de\/wp-content\/uploads\/Nicht-glaenzende-Metalle-SEM-EDX-300x231.jpg 300w, https:\/\/www.rjl-microanalytic.de\/wp-content\/uploads\/Nicht-glaenzende-Metalle-SEM-EDX-768x592.jpg 768w\" sizes=\"(max-width: 992px) 100vw, 992px\" \/>\t\t\t\t\t\t\t\t<\/a>\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-cbecf5d elementor-widget elementor-widget-heading\" data-id=\"cbecf5d\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h3 class=\"elementor-heading-title elementor-size-default\">Light Microscopy Underestimates the Quantity of Metallic Particles<\/h3>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-323dc4ca elementor-widget elementor-widget-text-editor\" data-id=\"323dc4ca\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>The following comparison with SEM-EDX shows just how serious the erroneous typification by light microscopy can be. The membrane as well as the result of optical particle analysis was provided to us by an automotive supplier. The comparison with SEM-EDX was carried out in our\u00a0<a class=\"unterstrichen\" href=\"\/en\/analysenservice-mit-iso-17025-akkreditierung\/\">accredited test laboratory.<\/a>\u00a0In this particular case, less than 1\/60 of the actual metal particles were detected by light microscopy.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-3d202fd elementor-widget elementor-widget-image\" data-id=\"3d202fd\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"image.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<a href=\"https:\/\/www.rjl-microanalytic.de\/wp-content\/uploads\/Vergleich-SEM-EDX-optische-Partikelanalyse.jpg\" data-elementor-open-lightbox=\"yes\" data-elementor-lightbox-title=\"Vergleich-SEM-EDX-optische-Partikelanalyse\" data-e-action-hash=\"#elementor-action%3Aaction%3Dlightbox%26settings%3DeyJpZCI6Mjc4NCwidXJsIjoiaHR0cHM6XC9cL3d3dy5yamwtbWljcm9hbmFseXRpYy5kZVwvd3AtY29udGVudFwvdXBsb2Fkc1wvVmVyZ2xlaWNoLVNFTS1FRFgtb3B0aXNjaGUtUGFydGlrZWxhbmFseXNlLmpwZyJ9\">\n\t\t\t\t\t\t\t<img decoding=\"async\" src=\"https:\/\/www.rjl-microanalytic.de\/wp-content\/uploads\/Vergleich-SEM-EDX-optische-Partikelanalyse.jpg\" title=\"Comparison-SEM-EDX-optical-particle analysis\" alt=\"Vergleich-SEM-EDX-optische-Partikelanalyse\" class=\"elementor-animation-float\" loading=\"lazy\" \/>\t\t\t\t\t\t\t\t<\/a>\n\t\t\t\t\t\t\t\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-dc6e9f4 elementor-widget elementor-widget-heading\" data-id=\"dc6e9f4\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"heading.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t<h3 class=\"elementor-heading-title elementor-size-default\">Our Recommendation to You<\/h3>\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t<div class=\"elementor-element elementor-element-430a7e4d elementor-widget elementor-widget-text-editor\" data-id=\"430a7e4d\" data-element_type=\"widget\" data-e-type=\"widget\" data-widget_type=\"text-editor.default\">\n\t\t\t\t<div class=\"elementor-widget-container\">\n\t\t\t\t\t\t\t\t\t<p>In applications where the reliable detection of metallic particles is critical for a component's functionality, e.g. electronical parts, we recommend particle analysis by the means of SEM-EDX. For routine analysis of component cleaning, the optical detection of metals should be completely eliminated and only the total number of particles should be considered instead. Talk to our\u00a0<a class=\"unterstrichen\" href=\"\/en\/company\/mitarbeiter-team\/\">experts<\/a>\u00a0and benefit from our many years of experience.<\/p>\t\t\t\t\t\t\t\t<\/div>\n\t\t\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/div>\n\t\t\t\t\t<\/div>\n\t\t<\/section>\n\t\t\t\t<\/div>","protected":false},"excerpt":{"rendered":"<p>The identification of metallic particles is an important requirement in cleanliness analysis. In recent years, the light-optical detection of metallic particles has commonly been performed by the means of gloss. On the basis of our laboratory experience, we have found that the light microscopic analysis often leads to incorrect typifications, which can be easily avoided by a material analysis using SEM-EDX.<\/p>","protected":false},"author":1,"featured_media":2002,"comment_status":"closed","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[9,11,12],"tags":[69,14,22,68,38,39,41,43,45,49,50],"class_list":["post-1390","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-innovative-analytik","category-analyse-technische-sauberkeit","category-elektronenmikroskopie-sem-edx","tag-analysen-mit-akkreditierung","tag-bauteilsauberkeit","tag-iso-16232","tag-prueflabor","tag-restschmutz","tag-restschmutzanalyse","tag-roentgenelementanalyse","tag-sauberkeitsanalyse","tag-sem-edx","tag-technische-sauberkeit","tag-vda-19"],"aioseo_notices":[],"_links":{"self":[{"href":"https:\/\/www.rjl-microanalytic.de\/en\/wp-json\/wp\/v2\/posts\/1390","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.rjl-microanalytic.de\/en\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/www.rjl-microanalytic.de\/en\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/www.rjl-microanalytic.de\/en\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/www.rjl-microanalytic.de\/en\/wp-json\/wp\/v2\/comments?post=1390"}],"version-history":[{"count":20,"href":"https:\/\/www.rjl-microanalytic.de\/en\/wp-json\/wp\/v2\/posts\/1390\/revisions"}],"predecessor-version":[{"id":10342,"href":"https:\/\/www.rjl-microanalytic.de\/en\/wp-json\/wp\/v2\/posts\/1390\/revisions\/10342"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/www.rjl-microanalytic.de\/en\/wp-json\/wp\/v2\/media\/2002"}],"wp:attachment":[{"href":"https:\/\/www.rjl-microanalytic.de\/en\/wp-json\/wp\/v2\/media?parent=1390"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/www.rjl-microanalytic.de\/en\/wp-json\/wp\/v2\/categories?post=1390"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/www.rjl-microanalytic.de\/en\/wp-json\/wp\/v2\/tags?post=1390"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}